Example of Tirneauuz tungsten-molybdenum ore dressing plant in the Caucasus

1 Introduction
Located in the Caucasus, Tirne Auz is a tungsten- molybdenum mining-selection joint venture.
1940 flotation production, the existing production capacity of 1200t / d, the amount of molybdenum is a gold production per year 3000t, tungsten metal content 2400t.
2. Deposits, ores and mining
Tierne Auz is a skarn or skarnized marble molybdenum-tungsten deposit and horn rock and granite molybdenum deposit. The proven ore reserves are 50 Mt, the tungsten and molybdenum grades are 0.65% WO 3 and 0.25% Mo, and the retained molybdenum metal reserves are 125 kt, of which the recoverable molybdenum metal is 65 kt.
The ore is classified into two types, silicate and carbonate, according to the type of associated gangue.
The main metal minerals in the skarn type ore are fine-grained inlaid (0.01~lmm) scheelite , tungsten-molybdenum-calcium ore and molybdenum ore present in surrounding rocks (hornblende, garnet, quartz, etc.). The ore has the highest content of molybdenum and tungsten trioxide. There are also copper , bismuth , gold, silver , selenium , hooves, fluorite and the like.
The distribution of molybdenum-containing minerals and molybdenum in the ore is: molybdenum ore 50%, molybdenum-tungsten ore 30%, molybdenum-containing scheelite 11%, and molybdenum-containing vermiculite 8%.
Mine used pit mining, crushing the stope, ore dressing plant with ropeway sent.
3. Mineral processing technology
Tierne Uz tungsten-molybdenum ore comprehensively recovers molybdenum, copper and tungsten, using copper-molybdenum mixed flotation; copper-molybdenum separation and copper selection; copper-molybdenum mixed flotation tailings flotation scheelite.
The copper-molybdenum mixed flotation and copper-molybdenum separation process is shown in Figure 1. The copper-molybdenum mixed float is selected from coarse grinding (60%~69%-200 mesh), one rough selection, one sweep selection, and two selective processes. The copper-molybdenum mixed concentrate was subjected to steaming heat treatment and a section (three fine bubbles) for re-grinding, and five times (third to seventh) were selected to obtain qualified molybdenum concentrate. After the copper-molybdenum sorting ore is mixed and floated, it is subjected to steaming heat treatment and molybdenum floating copper to obtain qualified copper concentrate.
Figure 1 Tirne Auz selection plant process
[next]
The process of the tungsten recovery circuit is shown in Figure 2. The sulphur concentrate is divided into three streams: the first one enters re-selection to obtain high-grade scheelite concentrate; the second one directly leaches phosphorus ; the third one is low-quality scheelite concentrate, which is sent to the water and metallurgical plant for treatment.
The white tungsten coarse concentrate is selected by steaming process, and the slurry is heated to 85~87 °C, and then treated with 2.7%~3% water glass solution for 60 min and then selected.
Figure 2 Tirne Auz recycling white tungsten process
4. Mineral processing agent
The mineral processing agent system is listed in the table below.
Table Tierner Auze Concentrator Pharmacy System
Work
Calcined soda
Butyl xanthate
Fatty acid
Transformer oil
Coal oil
Isodecenol
Sodium sulfide
Sodium cyanide
Water glass
Grinding
690
5
Molybdenum rough selection
5
50
Regrind
6
Molybdenum selection
     
50
50
5
130
Copper-molybdenum ore flotation:
Mixed rough selection
0.7
2
2
Sweep
0.3
30
Stir
350
White tungsten flotation:
Rough selection
40
41
Sweeping (I and II)
27
I selection
150
Steam heating
1880
Total consumption
730
10
68
10
52
48
80
5
2516
5, mineral processing indicators
The ore grade is 0.65% Mo, 0.25% WO 3 ; the ore processing capacity is 1200t/d, the grinding fineness is 60%-200 mesh; the molybdenum concentrate grade is 47.65% Mo, 0.416% WO 3 , the molybdenum recovery rate is 47.98%; The ore grade is 61.94% WO 3 , 3.56% Mo, the tungsten recovery rate is 22.23%; the white tungsten intermediate product grade is 44.41% WO 3 , 3.59% Mo, the tungsten recovery rate is 62.79%; the power consumption is 18.56kW·h/t ore, water: 2.208 m 3 /t mine, steel ball: 0.855kg / t mine, liner: 0.lkg / t mine.

FJZP-220 is Four Wheel ride On Laser Screed, it is mainly used in large area concrete construction, such as large workshop, airport, the plaza and so on. 

ride on four wheel laser screed


FURD ride on four wheel Laser Screed:

-Used high accuracy laser device, close loop control technology and precision integrated hydraulic system, and microcomputer automatic control.

-The flat and dual slope can be fully automatic controlled by the transmitter. For the complex floor which has high requirement for drainage, the 3-D floor processing system can be used.

-Steering, forward and reverse of the machine are all controlled by the integrated handles. Operation buttons and controller which are located on the one side of th seat, is user-friendly.


Four Wheel Ride On Laser Screed

Four Wheel Tide On Laser Screed,Four Wheel Ride On Concrete Laser Screed,Ride On Type Concrete Laser Screed,Cement Floor Leveling Machine

Jining Furuide Machinery Manufacturing Co., Ltd. , https://www.vibratoryroller.nl